1.1  Desizing: This process to remove the size material and increase the absorbency power of the fabric to make the fabric suitable for the next process is called Desizing.
Chemical Types:
 1. Detergent – 200gm
2. Caustic soda – 400gm
3. Water – 400 L
4. Hydrogen Peroxide – 600gm
5. Temperature - 70°c

At first mixed the chemical then run the machine 10 minutes at 70°c. After this process to proper clean the machine with 800 L water.
1.2 Neutral: Neutral is done to control the pH of this process pH must be checked. Some chemical are use for the process. At first Acetic Acid (100gm) with water 400 L to run the machine 5 minutes at 45°c. Then after this process to proper clean the machine with 800 L water for the next process.
1.3 Dyeing: This process by which is a textile material is to be changed physically or chemically, so that it looks mono uniform colored is called Dyeing.
Alfatex + Anticrease = 45°c – 5min
Dye Chemical = 55°c – 5min + Salt after 20min
Fixing Agent
 Softening Agent
 Rinsing Wash
Dain
1.4 Objects of dyeing:
1. The textile goods are dyed uniformly with single color.
2. To increase the attractiveness of the textile goods.
3. To make the fabric suitable for various usage.
4. To make textile goods suitable for decorative purposes.
Some necessary chemicals are needed for this process. Such as
1. Alfatex – 500gm
2. Anticrease – 500gm
Anticrease removes crease mark. The Belly Machine run 5 minute with chemical and water at 80°c temperature then add dyestuff.
 Indosol Scarlet BL – 350GM
 Rose RR – 66.25gm
 Red BA – 153.5gm
 Salt – 15kg
Those chemical are mixed in a bath. Those chemical are taken in a Belly Mache with 800 L water to run the machine 5 minute at 80°c temperature then check garments to match the shade.
1.5 Fixing: This is a very important process because it helps to carry dye in garments. It increases durability dye in the garments. For this process fixing agent such as hydrocol sun (300gm) and water is needed to run machine 5 minute at 40°c. Then after this process to proper clean the machine with 800 L water for the next process.
1.6 Enzyme: This process is done when the garments carry excess dye than the buyer requirement. But when garments carry light that time enzyme process is not necessary. For enzyme process Jak powder (150gm) and pocket clear (100gm) are needed with water to run the machine 5 minute at 40°c temperature. After this process to proper clean the machine with 800 L water.
1.7 Softener: Softener is used to soft the garments. For this process IMA and Acetic Acid are needed with water to run the machine 5 minute at 40°c temperature then garments out. After Finishing those process garments are taken out for finish dry process. Time, Temperature, Liquor Ratio must be controlled.
1.8 Garments dyeing process with vat dyes: The following process is suitable specially for garment dyeing. Typical recipe: Wetting agent = 0.5 – 1.0 g/l Sequestering agent = 1.0 - 2.0 g/l Leveling agent = 1.0 - 2.0 g/l Retarding agent – 5 - 7 g/l (If necessary use in hot dyes) Dyes = 7% (owf) Caustic soda = 5 %(according to vender recommendation) Hydros (sodium hydrosulfite) = 5%( according to vender recommendation) Temperature = 70°c - 80°c Time = 30 – 50 min M: L = 1:10
Procedure:
1. First, settle dye bath with substrate at 40°c and wetting, sequestering agent, leveling, retarding agent (if necessary) and then run for 5 – 10 min.
2. Add dyes according to substrate weight and run the bath for 5 min.
3. Add 2/3 of caustic soda requirements and run for 5 min.
4. Raise the temperature to 70 – 80 at 2-3c/min and run for 5 min.
5. Add Sodium hydrosulfite (hydroz) to the bath with rest 1/3 amount of caustic requirements.
6. Run the bath for 30 min and maintain reduction by checking with vat reduction paper.
7. Overflow rinse until with cold water.
1.9 Oxidation: After dyeing cycle penetrated and distributed dye molecules are oxidized to convert insoluble form into the fiber. The oxidation process can be done in contact of air or other oxidizing agent. For example, the oxidation process can be carried out treating the dyed goods with 0.5 – 1.0 g/l hydrogen 35% at 30 – 35 for 10 min.
1.9.1 Soaping:
Detergent = 1.0 – 2.0 g/l
Soda ash = 1- 2 g/l
Glucose = 95 – 100c
Time = 15 – 30 min
M: L = 1: 10 – 1: 20
The rinse the goods with cold-hot-cold water successively.
1.9.2 Softening:
1. That the good with 1.0 – 2.0% softening agent at 10 min.
2. Drop
3. Finally dry the goods uses.

Comments

Popular posts from this blog

"মার্চেন্ডাইজিং এ টু জেড"

আগের পোস্টের ধারাবাহিকতা অনুসারে আজকে বায়িং হাউজ এবং মার্চেন্ডাইজিং-এ সফলতা অর্জনের জন্য প্রয়োজনীয় দক্ষতা কি কি থাকা উচিৎ এগুলো নিয়ে বিস্তারিত আলোচনা করা হয়েছে। আগের মার্চেন্ডাইজিং এর উপর করা আর্টিকেলে " এপারেল মার্উচেন্ডাজিং" এর উপর বিশদভাবে আলোচনা করা হয়েছিল।   বায়িং হাউজঃ - বাইং হাউজ হচ্ছে আমাদের দেশে রপ্তানিমুখী পোশাক শিল্পের এক ধরনের ব্যবসা । যে ব্যবসাটাকে আমরা বলে থাকি ১০০ % এক্সপোর্ট ওরিয়েন্টেড বিজনেস । এখানে বায়িং হাউজ শব্দটি   বলতে বুঝায় , " বাই" মানে কেনা আর  " হাউজ" শব্দটি কোন ব্যবসা প্রতিষ্ঠান অর্থে ব্যবহৃত হচ্ছে । অর্থাৎ বায়িং হাউজ একটা ব্যবসা প্রতিষ্ঠান যেটা মুলত ট্রেডিং হিসাবে কাজ করে থাকে । বায়িং হাউজের মূল কাজ হচ্ছে   বায়ারের সাথে যোগাযোগ করা এবং অর্ডার নেগোসিয়েট করা । এবং পরিশেষে অর্ডার কনফার্ম হয়ে গেলে সেটা কোন ফ্যাক্টরির মাধ্যমে এক্সিকিউট করিয়ে অর্ডারটি শিপমেন্টের ব্যবস্থা করাই   হল বায়িং হাউজের কাজ । আর অর্ডার যখন বায়িং হাউজের হাত ধরে ফ...

MS office Shortcut Keys

Shortcuts Keys Operation Ctrl+X Cut Ctrl+C Copy Ctrl+V Paste Ctrl+Z Undo Ctrl+Y Redo Ctrl+S Save Ctrl+P Print Shortcuts for moving around easily / quickly in Word Home Beginning of line End End of line Ctrl + Home Go to start of document Ctrl + End Go to end of document Right Arrow Right one character Left Arrow Left one character Ctrl+Right Arrow Right one word Ctrl+Left Arrow Left one word Up Arrow Up one line Down Arrow Down one l...

কতো GSM এর জন্য কতো Count (Ne) সুতা লাগবে

কি ভাবে বের করবো কতো GSM এর জন্য কতো Count (Ne) লাগবে, এটার সিদ্ধান্ত দেয়া এক জন টেক্সটাইল ইঞ্জিনিয়ার বা ফেব্রিক ইঞ্জিনিয়ার এর মুল কাজ। এটি অভিজ্ঞার ফসল, তার পরও কিছু টিপস আছে যা ফোলো করলে আরো সহজে কাজের এর প্লান করা যায় । জেনে নি কিভাবে বের করবেন আপনার কাপড় এর জন্য কতো কাউন্ট এর সুতা দিলে কতো GSM আসবে : S/J = 4300 ÷ GSM Pique=5200 ÷ GSM Fleece=7200 ÷ GSM Interlock=7200 ÷ GSM 1X1 Rib=6000 ÷ GSM Lacost=5500 ÷ GSM 2X2 Rib=6250 ÷ GSM Terry =6240 ÷ GSM এখানে GSM এর ঘরে বায়ার যে GSM চাবে তা ওই GSM এর ঘরে বসিয়ে দিলে আপনি ওই GSMএর কাপড় তৈরি করতে কোন কাউন্ট এর সুতা লাগবে তা বের করতে পারবেন ! S/J=(0.141x GSM)+50.22 Pique= (0.146 x GSM )+57.16 Dabol Lacost= (0.167 x GSM )+64.36 1X1 Rib= (0.123 x GSM )+54.57 Interlock= (0.206 x GSM )+80.56 Lycra 1X1 Rib= (0.119 x GSM )+59.12 Lycra 2X2 Rib = (0.108 x GSM)+56.62 Relation between count and GSM: জেনে নিন কাউন্ট এর সাথে GSM এর সম্পর্ক অথবা কি কাউন্ট দিলে কোন কাপড় এর জন্য কি GSM আসবে smile emoticon নিটিং কাজ করা এক জন...